金属间表面磨损问题--请教

[复制链接]
发表于 2009-1-12 16:39:01 | 显示全部楼层 |阅读模式
SS430不锈钢钢板和HQ SS302螺钉配合安装,拆下螺钉发现钢板接触面磨损--如图。
/ C9 k8 P) j4 U# \" a% a8 x磨损将产生颗粒,影响产品性能。1 \8 B/ K. G0 I/ b8 n
不知道钢板换成铝合金板是否能避免表面磨损的问题?

本帖子中包含更多资源

您需要 登录 才可以下载或查看,没有帐号?注册会员

x
回复

使用道具 举报

 楼主| 发表于 2009-2-20 09:08:31 | 显示全部楼层
Galling is the welding of 2 mating parts due to excessive friction during fastenings. This can reduce the production yield of HDD. ( D0 d' v2 a+ V, s" b" U& _
1 D% v: R& X3 P' x. j( ]
来自网络:% K* D  V& I( ?; P, }3 e3 _: x! q; ]
Anti-Galling Fasteners
. Q0 G" }# h* g& n Unisteel pioneered anti-galling technologies in late 1999 to overcome what is termed as galling in the HDD industries. ' Z+ W! |; I8 y8 w: m3 ]; g" ~) L

% y5 `& `* ]2 A7 WGalling is the welding of 2 mating parts due to excessive friction during fastenings. This can reduce the production yield of HDD. Unisteel uses the CAMTRONIC and UNITRONIC materials to produce such anti-galling fasteners for HDD industry. Unisteel is amongst the leading manufacturer with technologies to produce such fasteners.
回复 支持 反对

使用道具 举报

发表于 2009-2-20 16:14:48 | 显示全部楼层
只能减轻,不能避免
回复 支持 反对

使用道具 举报

 楼主| 发表于 2009-2-20 16:32:20 | 显示全部楼层
原帖由 滕刚 于 2009-2-20 16:14 发表
1 _  p" h+ l; n# O只能减轻,不能避免

6 _0 z  w: z, g
7 e+ h5 d2 C) P绝对的避免是不可能的了,镀镍或者镀聚合物复合涂层能改善很多,只是成本问题又出来了..
回复 支持 反对

使用道具 举报

您需要登录后才可以回帖 登录 | 注册会员

本版积分规则

小黑屋|手机版|Archiver|机械社区 ( 京ICP备10217105号-1,京ICP证050210号,浙公网安备33038202004372号 )

GMT+8, 2024-11-26 20:24 , Processed in 0.054054 second(s), 17 queries , Gzip On.

Powered by Discuz! X3.4 Licensed

© 2001-2017 Comsenz Inc.

快速回复 返回顶部 返回列表